A Puddle Platter from Puddle Cabochons? Sounds Odd! Fused Glass Project Tutorial.

Описание к видео A Puddle Platter from Puddle Cabochons? Sounds Odd! Fused Glass Project Tutorial.

I've had some black and white fused glass puddle cabochons for ages. Always wondered what to do with them and now was the time. Of course, a platter. What else should a fused glass artist make?

Plenty, actually. But I decided a platter would be cool. I hope you enjoy this project tutorial and please let me know your thoughts..

#JeffPritchard (Australian Glass Artist)

🔴 Join Membership -    / @rocketroseart  
This will open YouTube in a browser so you can join.

🔴 Subscribe -    / @rocketroseart  

⏱️ Chapters ⏱️
0:00 Intro & Details
2:23 Design & Materials
4:48 Assembly of Feature Bar
5:16 Full Fuse of Feature Bar
6:24 Coldworking Feature Bar
8:50 Cutting Glass for Part Sheet
9:53 Assembling Part Sheet
12:49 Fusing Part Sheet & Result
14:04 Coldworking Part Sheet
16:18 Cutting Glass & Final Assembly
17:16 Full Fuse of Final Assembly & Result
18:56 Coldworking & Frit Application
19:56 Fusing Frit & Result
23:42 Sandblasting
24:08 Final Slump Fuse

📌 Other Glass Fusing Videos
🎥 Fused Glass Playlists -    / @rocketroseart  

💥 Full Fuse Firing Schedule (feature bar)
1 - 222 C (432 F) up to 535 C (995 F), hold 30 minutes
2 - 333 C (632 F) up to 670 C (1238 F), hold 30 minutes
3 - Full up to 805 C (1480 F), hold 10 minutes
4 - Full down to 482 C (900 F), hold 60 minutes
5 - 65 C (149 F) down to 425 C (797 F), no hold
6 - 132 C (270 F) down to 371 C (700 F), no hold

💥 Contour Fuse Firing Schedule (part sheet)
1 - 222 C (432 F) up to 535 C (995 F), hold 30 minutes
2 - 333 C (632 F) up to 670 C (1238 F), no hold
3 - Full up to 790 C ( F), hold 10 minutes
4 - Full down to 482 C (900 F), hold 120 minutes
5 - 65 C (149 F) down to 425 C (797 F), no hold
6 - 132 C (270 F) down to 371 C (700 F), no hold

💥 Full Fuse Firing Schedule (whole piece)
1 - 222 C (432 F) up to 535 C (995 F), hold 60 minutes
2 - 333 C (632 F) up to 670 C (1238 F), hold 60 minutes
3 - Full up to 805 C (1480 F), no hold
4 - Full down to 482 C (900 F), hold 60 minutes
5 - 65 C (149 F) down to 425 C (797 F), no hold
6 - 132 C (270 F) down to 371 C (700 F), no hold

💥 Fuse Firing Schedule (clear frit)
1 - 222 C (432 F) up to 535 C (995 F), hold 60 minutes
2 - 333 C (632 F) up to 670 C (1238 F), no hold
3 - Full up to 780 C ( F), hold 10 minutes
4 - Full down to 482 C (900 F), hold 120 minutes
5 - 65 C (149 F) down to 425 C (797 F), no hold
6 - 132 C (270 F) down to 371 C (700 F), no hold

💥 Slump Firing Schedule (final piece)
1 - 167 C (333 F) up to 630 C (1166 F), hold for 5 minutes
2 - Full down to 482 C (900 F), hold 120 minutes
3 - 65 C (149 F) down to 425 C (797 F), no hold
4 - 132 C (270 F) down to 371 C (700 F), no hold